Rule of JAS Standard DARI SALAH SATU PERUSAHAAN YANG BERGERAK DI BIDANG KAYU LAPIS (PLYWOOD)

1.Bonding strength Test

1.a. The sample divides into two parts, which have the bonding test at the mill Lab and MAL (Mutu Agung Lestari).

1.b.If the inspector found delamination in ripping test by hand, the inspector has to take 1 sheet of the additional sample for the laboratory and MAL.

1.c. The bonding strength test shall conform to JAS Standard.

2.Standard of Judgement

Consecutive boiling test (Repetition boiling test):

Rate of pass Judg  
More than 90% PASS Pulling strength, wood destructive rate
Less than 70% NG
More than 70%, less than 90% Re-test Result re-test more than 90% then pass, less than 90% then NG

 

Hope usefull..🙂

 

 

 

 

 

 

Perihal Rudi Hermawan
Ku dilahirkan di daerah terpencil, jauh dari keramaian. Beberapa puluh tahun kemudian baru tahu keramaian kota. Dan dari keadaan tersebut sedikit banyak mewarnai gaya tuturku dalam tulisan. Tapi, siapapun itu orangnya yang membuat tulisan, tidak terlalu perlu untuk diperhatikan, yang perlu diperhatikan adalah isi pesan dari tulisan itu. Semoga bermanfaat.. :)

Tinggalkan Balasan

Isikan data di bawah atau klik salah satu ikon untuk log in:

Logo WordPress.com

You are commenting using your WordPress.com account. Logout / Ubah )

Gambar Twitter

You are commenting using your Twitter account. Logout / Ubah )

Foto Facebook

You are commenting using your Facebook account. Logout / Ubah )

Foto Google+

You are commenting using your Google+ account. Logout / Ubah )

Connecting to %s

%d blogger menyukai ini: